水性厚板浆印不厚怎么办?
1、选择浆料很重要、厚板浆有PU厚板浆,有普通厚板浆
2、网板一定要晒厚的网板,或把网板的四个角垫高起来
厚板浆调配比例
① 厚板浆(透明)+0.5%PTF增稠剂(华樾)印厚些
② 盖面:厚板浆(白)(80%)+厚板浆(透明)(20%)+0.5%PTF增稠剂(华樾),印3次
③ 红色厚板:厚板浆(白)(20%)+厚板浆(透明)(80%)+A014大红(劳安)+0.5%PTF增稠剂(华樾),印3次
工艺流程
1. 丝网选用80-100目厚板,用丝印硬方刀75度刮印, 以厚板浆(透明)打底2-3次
2. 将厚板浆(白),厚板浆(透明),高温色浆搅拌匀印2-3次
3. 24-48小时自然干燥,或150-180度焙烘1-3分钟
What should I do if the Waterborne thick plate pulp printing is not thick?
Product name
Waterborne thick plate pulp (glossy)
Packing
25KG/drum for white, 20KG/drum for clear
Storage
6 months in cool place
Application
Suitable for cotton, polyester etc
Features
1. High elasticity
2. High fastness
3. SGS detecting passed, no PVC, no heavy metal, no NPEOs
Mix proportion
1 Waterborne thick plate pulp(Clear)+0.5% PTF Thickener(HY Chemical) printing thickness
2 cover: Waterborne thick plate pulp(White) (80%) + Waterborne thick plate pulp(Clear) (20%) + 0.5% PTF Thickener(HY Chemical), printed 3 times
3 red: Waterborne thick plate pulp(White) (20%) + Waterborne thick plate pulp(Clear) (80%) + Pigment Red A014(Laoan Chemical)+ 0.5% PTF Thickener(HY Chemical), printed 3 times
Printing process
1. Printing with Waterborne thick plate pulp(Clear) for 2-3 times
2. Mixing with Waterborne thick plate pulp(White), Waterborne thick plate pulp(Clear), pigment and stirring them evenly.
3. Printing again for 3-4 times (3-4 scrapes per time).
4. Drying it in room temperature, or baking for 1-3 minutes under 150-180℃
5. Finish.